Oct 16, 2021

Tin bronze is a bronze with tin as the main alloying element. It has high mechanical properties, anti-wear properties and corrosion resistance, and is easy to cut. The tin content is generally between 3 to 14%, and sometimes phosphorus, lead, zinc and other elements are added. Adding phosphorus can improve fluidity and wear resistance; adding lead can improve machinability and wear resistance; adding zinc can improve casting performance.

The tin-bronze copper sleeve is prone to severe shrinkage, porosity, hot cracking and serious segregation during casting. To solve the problem of shrinkage and porosity, copper alloys need to be smelted in a strong oxidizing atmosphere. Our factory uses 0.3~0.4MPa dry compressed air to blow into the copper liquid to increase the amount of oxidation to maximize hydrogen removal, and then remove the copper alloy in the copper liquid. Oxygen, we add phosphorus copper to deoxidize three times, once after the pure copper melts. Add the bottom of the package twice after the furnace, and add deoxidation in the package three times, but the phosphorous copper should not exceed 1.5%, otherwise it will reduce the strength and toughness and make the alloy brittle. The deoxidation must be sufficient and the slag must be clean. Otherwise, the deoxidation product will easily contaminate the copper liquid, and the copper liquid will easily form pores and slag holes after solidification. 0.03~0.05% of mixed rare earth must be added.

In terms of modeling, we added 2% sawdust to the core sand, and wrapped a circle of straw rope in the core bone to increase the concession of the sand core and prevent the casting from being blocked due to solidification and shrinkage.

Due to the large difference in the density and melting point of copper, tin and lead, segregation is easy to occur. The copper liquid needs to be fully stirred before pouring, and it needs to be cooled to a certain temperature within a specified time after pouring, so that the lead will not sink and the tin will solidify before it can precipitate.

www.cn-czpufa.com

Send Inquiry